The Sarlink ME-2600 Series is a super high flow high performance thermoplastic elastomer series, available in BLK, designed for automotive exterior molded applications, including window encapsulation. Sarlink ME-2675B is a medium hardness, low density, resilient, UV stabilized, super high flow injection molding grade delivering excellent aesthetics with good adhesion to glass with primer. |
General Information | |
---|---|
Features |
|
Uses |
|
RoHS Compliance |
|
Appearance |
|
Forms |
|
Processing Method |
|
Physical | Nominal Value | Unit | Test Method |
---|---|---|---|
Density | 0.938 | g/cm³ | ISO 1183 |
Melt Mass-Flow Rate (MFR) (190°C/2.16 kg) | 18 | g/10 min | ASTM D1238 |
Hardness | Nominal Value | Unit | Test Method |
---|---|---|---|
Durometer Hardness | ISO 868 | ||
Shore A, 1 second, injection molding | 77 | ISO 868 | |
Shore A, 5 seconds, injection molding | 74 | ISO 868 | |
Shore A, 15 seconds, injection molding | 73 | ISO 868 |
Elastomers | Nominal Value | Unit | Test Method |
---|---|---|---|
Tensile Stress | ISO 37 | ||
Transverse flow : 100% strain | 2.55 | MPa | ISO 37 |
Flow : 100% strain | 2.79 | MPa | ISO 37 |
Tensile Strength | ISO 37 | ||
Transverse flow : Fracture | 10.5 | MPa | ISO 37 |
Flow : Fracture | 9.20 | MPa | ISO 37 |
Tensile Elongation | ISO 37 | ||
Transverse flow : Fracture | 790 | % | ISO 37 |
Flow : Fracture | 730 | % | ISO 37 |
Tear Strength | ISO 34-1 | ||
Transverse flow | 33 | kN/m | ISO 34-1 |
Flow | 33 | kN/m | ISO 34-1 |
Compression Set | ISO 815 | ||
23°C, 22 hr | 23 | % | ISO 815 |
70°C, 22 hr | 45 | % | ISO 815 |
90°C, 70 hr | 69 | % | ISO 815 |
Aging | Nominal Value | Unit | Test Method |
---|---|---|---|
Change in Tensile Strength in Air - Across Flow | ISO 188 | ||
110°C, 1008 hr | -2.0 | % | ISO 188 |
125°C, 168 hr | -7.0 | % | ISO 188 |
Changes in tensile stress upon fracture in air- Transverse flow | ISO 188 | ||
110°C, 1008 hr | 0.50 | % | ISO 188 |
125°C, 168 hr | -1.6 | % | ISO 188 |
Change in Shore Hardness in Air | ISO 188 | ||
Shao A, 110°C, 1008 hr | 1.9 | ISO 188 | |
Shao A, 125°C, 168 hr | 2.2 | ISO 188 |
Fill Analysis | Nominal Value | Unit | Test Method |
---|---|---|---|
Apparent Viscosity (200°C, 206 sec^-1) | 137 | Pa·s | ASTM D3835 |
Additional Information |
---|
Good adhesion to glass with primer |
Legal statement |
---|
The information and recommendations contained in this bulletin are, to the best of our knowledge, accurate and reliable but no guarantee of their accuracy is made. All products are sold upon condition that purchasers shall make their own tests to determine the suitability of such products for their particular purposes and uses and purchaser assumes all risks and liability for the results of use of the products, including use in accordance with seller's recommendations. Nothing in this bulletin constitutes permission or a recommendation to practice or use any invention covered by any patent owned by this company or others. There is no warranty of merchantability and there are no other warranties for the products described. For detailed Product Stewardship information, please contact us. Any product of Teknor Apex, including product names, shall not be used or tested in medical or food contact applications without the prior written acknowledgement of Teknor Apex as to the intended use. Please note that some products may not be available in one or more countries. |
Injection | Nominal Value | Unit | |
---|---|---|---|
Rear Temperature | 170 - 190 | °C | |
Middle Temperature | 175 - 195 | °C | |
Front Temperature | 180 - 205 | °C | |
Nozzle Temperature | 180 - 205 | °C | |
Processing (Melt) Temp | 180 - 205 | °C | |
Mold Temperature | 15 - 40 | °C | |
Injection Pressure | 1.38 - 6.89 | MPa | |
Injection Rate | Fast | ||
Back Pressure | 0.172 - 0.862 | MPa | |
Screw Speed | 50 - 120 | rpm | |
Cushion | 3.81 - 25.4 | mm |
Injection instructions |
---|
Drying is not necessary. However, if moisture is a problem, dry the pellets for 2 to 4 hours at 180°F (80°C). |
Resin Grade | Manufacturer | Category | Trademark |
---|---|---|---|
RTP 301 | RTP Company | PC | RTP |
ADMER™ QF500A | Mitsui Chemicals America, Inc. | PP, Unspecified | ADMER™ |
BioCeres® BC-LBI02 | FuturaMat | Biodeg Polymers | BioCeres® |
Kingfa PP-KF06 | Kingfa | PP, Unspecified | Kingfa |
POLYblend PC/ABS C65F | Polykemi AB | PC+ABS | POLYblend |